Tensile Properties

Tensile Data, Plate

Test Temperature Ultimate Tensile Strength 0.2% Yield Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 200.5 1382 167.8 1157 20.6
800 427 173.1 1193 149.0 1027 22.6
1000 538 170.2 1173 145.9 1006 21.8
1200 649 162.5 1120 139.9 965 25.1
1400 760 117.3 809 104.9 723 12.1
1600 871 42.2 291 34.3 236 68.0
1800 982 14.1 97 9.6 66 129.9

Mill Annealed + 1325°F/8h/Furnace Cool to 1150°F/8h/Air Cool
Total time: 18 hours
RT= Room Temperature

Tensile Data, Sheet

Test Temperature Ultimate Tensile Strength 0.2% Yield Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 203.6 1404 174.7 1205 18.4
800 427 176.2 1215 155.4 1071 21.3
1000 538 172.3 1188 150.2 1036 20.7
1200 649 164.1 1131 144.3 995 16.3
1400 760 114.8 792 103.8 716 6.9
1600 871 39.9 275 34.0 234 81.8
1800 982 13.7 94 9.7 67 175.6

Mill Annealed + 1325°F/8h/Furnace Cool to 1150°F/8h/Air Cool
Total time: 18 hours

Top