Tensile Data

Sheet (AMS 5598)

Test Temperature Yield Strength
0.2% Offset
Ultimate Tensile
Strength
Elongation
°F °C ksi MPa ksi MPa %
RT RT 141.1 975 192.2 1325 23.6
1000 538 124.9 860 162.1 1120 22.2
1200 649 121.1 835 143.6 990 5.8
1400 760 92.0 635 94.3 650 2.5
1600 871 43.1 295 52.1 360 8.0
1800 982 9.1 63 16.6 115 42.0

RT=Room Temperature