HAYNES® Waspaloy Sheet, Age Hardened*
Temperature |
Creep |
Approximate Initial Stress to Produce Specified Creep in |
100h |
1,000h |
°F |
°C |
% |
ksi |
MPa |
ksi |
MPa |
1200 |
649 |
1 |
81 |
558 |
67 |
462 |
R |
92 |
634 |
80 |
552 |
1300 |
704 |
1 |
63 |
434 |
46 |
317 |
R |
75 |
517 |
57 |
393 |
1400 |
760 |
1 |
41 |
283 |
28 |
193 |
R |
53 |
365 |
35 |
241 |
1500 |
816 |
1 |
25 |
172 |
16 |
110 |
R |
32 |
221 |
20 |
138 |
1600 |
871 |
1 |
15 |
103 |
7.0 |
48 |
R |
19 |
131 |
10 |
69 |
1700 |
927 |
1 |
6.4 |
44 |
3.0 |
21 |
R |
10 |
69 |
4.8 |
33 |
*Samples were age hardened by treating at 1825°F (995°C)/2 Hr./AC + 1550°F (845°C)/4 Hr./AC + 1400°F (760°C)/16 Hr./AC