Baseline Tensile Properties at RT and ET; Residual Tensile Properties at
Room Temperature and Exposure Temperature
Condition |
Test Temperature |
0.2% Yield Strength |
Ultimate Tensile Strength |
4D Elongation |
°F |
°C |
ksi |
MPa |
ksi |
MPa |
% |
Solution Annealed |
RT |
RT |
83.6 |
576 |
151.4 |
1044 |
38.7 |
Age Hardened* |
RT |
RT |
116.8 |
805 |
178.6 |
1231 |
17.3 |
1200 |
649 |
103.1 |
711 |
169.6 |
1169 |
18.0 |
1400 |
760 |
111.6 |
769 |
138.2 |
953 |
28.4 |
1500 |
816 |
100.6 |
694 |
113.5 |
783 |
32.0 |
1600 |
871 |
78.1 |
538 |
87.9 |
606 |
30.0 |
Age Hardened* + 1200°F/8000h |
RT |
RT |
150.7 |
1039 |
188.5 |
1300 |
5.3 |
1200 |
649 |
129.7** |
894** |
182.6 |
1259 |
8.1** |
Age Hardened* + 1400°F/8000h |
RT |
RT |
151.6** |
1045** |
173.9** |
1199** |
0.1 |
1400 |
760 |
88.2 |
608 |
126.8 |
874 |
30.1** |
Age Hardened* + 1500°F/8000h |
RT |
RT |
113.5 |
783 |
156.6 |
1080 |
1.4 |
1500 |
816 |
58.2 |
401 |
88.5 |
610 |
26.8 |
Age Hardened* + 1600°F/8000h |
RT |
RT |
83.3 |
574 |
122.9 |
847 |
2.0 |
1600 |
871 |
36.3 |
250 |
60.9 |
420 |
33.0 |
*Aged hardened at 2050°F (1121°C)/30 MAT/AC + 1650°F (899°C)/4H/AC
**Limited data