Condition |
Test Temperature |
0.2% Yield Strength |
Ultimate Tensile Strength |
4D Elongation |
°F |
°C |
ksi |
MPa |
ksi |
MPa |
% |
Solution Annealed |
RT |
RT |
58 |
400 |
120.1 |
828 |
53.3 |
Age Hardened* |
RT |
RT |
93.1 |
642 |
154.2 |
1063 |
36.9 |
1200 |
649 |
78.2 |
539 |
132.3 |
912 |
38.6 |
1400 |
760 |
79.2 |
546 |
100 |
689 |
29.5 |
1500 |
816 |
69.3 |
478 |
77.9 |
537 |
36.9 |
1600 |
871 |
42.2 |
291 |
49.4 |
341 |
61.2 |
Age Hardened* + 1200°F/8000h |
RT |
RT |
113.3 |
781 |
176.8 |
1219 |
28.7 |
1200 |
649 |
96.7** |
667** |
149.2** |
1029** |
31.3** |
Age Hardened* + 1400°F/8000h |
RT |
RT |
83.3 |
574 |
151.3 |
1043 |
24.8 |
1400 |
760 |
60.9 |
420 |
83.7 |
577 |
36.4 |
Age Hardened* + 1500°F/8000h |
RT |
RT |
77.5 |
534 |
132.8 |
916 |
23 |
1500 |
816 |
42 |
290 |
58.6 |
404 |
37 |
Age Hardened* + 1600°F/8000h |
RT |
RT |
54.9 |
379 |
115.7 |
798 |
37.8 |
1600 |
871 |
38.4 |
265 |
25.5 |
176 |
49.1 |
* Samples were age hardened by treating at 1472°F for 8 hours and air cooling.
** Limited data