Tensile Properties

Hot-Rolled and Solution-annealed Plate

Test Temperature 0.2% Yield Strength Ultimate Tensile Strength Elongation
°F °C ksi MPa ksi MPa %
RT RT 70.1 483 143.8 991 50.6
1000 538 45.7 315 120.6 832 60.3
1200 649 45.1 311 121.6 838 62.8
1400 760 43.6 301 84.1 580 85.6
1600 871 37.1 256 49.5 341 97.9
1800 982 19.2 132 27.2 188 102.6
2000 1093 9.6 66 13.9 96 87.1

Cold-Rolled and Solution-annealed Sheet

Test Temperature 0.2% Yield Strength Ultimate
Tensile Strength
Elongation
°F °C ksi MPa ksi MPa %
RT RT 70.1 483 142.4 982 50.9
1000 538 44.8 309 117.4 809 58.8
1200 649 44.8 309 119.1 821 58.6
1400 760 43.8 302 81.6 563 81.8
1600 871 37.8 261 47.0 324 103.9
1800 982 18.2 125 25.4 175 81.0
2000 1093 8.5 59 12.4 85 49.7