Haynes International
Investor Relations
Customer Portal
English
日本語
中文
español
800.354.0806
765.456.6012
The Home of HASTELLOY® and HAYNES® Alloys
When autocomplete results are available use up and down arrows to review and enter to select.
Our Company
Company Overview
Locations and Directions
Investor Relations
Corporate Governance
Corporate Governance Guidelines
Corporate Policies
Human Trafficking Policy
Human Rights Policy
Conflicts Minerals Policy
Cancellation Policy
Anti-Harassment Policy
Anti-Corruption Policy
Health, Safety, Environmental, and Quality Policy
Energy Policy
Code of Business Conduct and Ethics
Suppliers and Third Party Intermediaries
EthicsPoint Whistleblower Hotline
Conduct and Ethics Compliance
Directors and Executive Officers
Composition of Board Committees
Board Committee Charters
Sustainability
Environmental
Social
Governance
Our Positive Impact
Health, Safety, Environmental, and Quality
Health, Safety, Environmental, and Quality Policy
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Energy Policy
Accreditations and Approvals
REACh
Trademarks
Our Heritage
Our Founder, Elwood Haynes
Our Company History
Our Milestones
Our Contributions to History
Careers
News
Markets
Aerospace
Power Generation
Chemical Processing
Emerging Technologies
Other Markets
Alloys
Alloy Portfolio
High-temperature Alloys
HAYNES® 25 alloy
HAYNES® 75 alloy
HAYNES® 188 alloy
HAYNES® 214® alloy
HAYNES® 230® alloy
HAYNES® 233™ alloy
HAYNES® 242® alloy
HAYNES® 244® alloy
HAYNES® 263 alloy
HAYNES® 282® alloy
HAYNES® 556® alloy
HAYNES® 617 alloy
HAYNES® 625 alloy
HAYNES® 625SQ® alloy
HAYNES® 718 alloy
HAYNES® HR-120® alloy
HAYNES® HR-160® alloy
HAYNES® HR-224® alloy
HAYNES® HR-235® alloy
MULTIMET® alloy
HAYNES® NS-163® alloy
HAYNES® R-41 alloy
HASTELLOY® S alloy
HASTELLOY® W alloy
HAYNES® Waspaloy alloy
HASTELLOY® X alloy
HAYNES® X-750 alloy
Corrosion-resistant Alloys
HASTELLOY® B-3® alloy
HASTELLOY® C-4 alloy
HASTELLOY® C-22® alloy
HASTELLOY® C-22HS® alloy
HASTELLOY® C-276 alloy
HASTELLOY® C-2000® alloy
HASTELLOY® G-30® alloy
HASTELLOY® G-35® alloy
HASTELLOY® HYBRID-BC1® alloy
HASTELLOY® N alloy
ULTIMET® alloy
Titanium Alloy
HAYNES® Ti-3Al-2.5V alloy
Alloy Nominal Compositions
Product Forms
Sheet and Plate
Wire and Welding
Pipe and Tubing
Bar and Billet
Fittings and Flanges
Welding and Fabrication
Welding and Fabrication Overview
Wire and Welding Product Forms
Hot-working
Cold-working
Welding and Joining
Heat Treatment
Machining
Grinding
Descaling and Pickling
Welding SmartGuide
Welding and Fabrication Brochure
Corrosion Guide
Introduction
Alloy Backgrounds
Alloy Groups
Metallurgy
Corrosive Environments
Wear Background
Abrasion
Erosion
Metal‐to‐Metal Sliding Wear
Corrosion Alloy Manual
Alloy Innovation
Alloy Development
Alloy Manufacturing
Alloy Technical Support
Specifications and Codes
Accreditations and Approvals
MSDS/Safety Data Sheets
Trademarks
Technical Library
Sales and Service
Sales and Service
Sales Office and Service Center Locations
Request for Quote
Terms and Conditions of Sale
Nickel Surcharges
Cancellation Policy
Export Compliance Policy Letter
Due Diligence
Incoterms®
Alloys and Products Brochure
Processing Capabilities
Abrasive Saw Cutting
Bar Saw Cutting
Laser Cutting
Near-net Shaped Cut Parts
Plasma Cutting
Precision Shearing
Virtek® Laser QC®
Waterjet Cutting
Contact
Sales
Technical Support
Investor Relations
Careers
General Information
HAYNES® 188 alloy
Home
Alloys
Alloy Portfolio
High-temperature Alloys
HAYNES® 188 alloy
Physical Properties
HAYNES® 188 alloy
Principal Features
Nominal Composition
Creep and Stress-Rupture Strength
Tensile Properties
Hardness Data
High-Temperature Hardness
Impact Strength Properties
Thermal Stability
Physical Properties
Low Cycle Fatigue Properties
Oxidation Resistance
Hot Corrosion Resistance
Sulfidation Resistance
Fabrication Characteristics
Welding
Machining
Specifications and Codes
Disclaimer
Alloy Brochure
ASP.sfctrlpresentation_openaccessdataprovider_7b98424546ba62e18cdfff0000376e70_ascx
HAYNES® 188 alloy
Principal Features
Nominal Composition
Creep and Stress-Rupture Strength
Tensile Properties
Hardness Data
High-Temperature Hardness
Impact Strength Properties
Thermal Stability
Physical Properties
Low Cycle Fatigue Properties
Oxidation Resistance
Hot Corrosion Resistance
Sulfidation Resistance
Fabrication Characteristics
Welding
Machining
Specifications and Codes
Disclaimer
Alloy Brochure
Physical Properties
Physical Property
British Units
Metric Units
Density
RT
0.324 lb/in
3
RT
8.98 g/cm
3
Melting Temperature
2400-2570°F
-
1315-1410°C
-
Electrical Resistivity
RT
39.6 µohm-in
RT
101.0 µohm-m
200°F
40.3 µohm-in
100°C
103.0 µohm-m
400°F
41.5 µohm-in
200°C
105.0 µohm-m
600°F
42.7 µohm-in
300°C
107.7 µohm-m
800°F
43.8 µohm-in
400°C
110.5 µohm-m
1000°F
44.7 µohm-in
500°C
112.7 µohm-m
1200°F
45.6 µohm-in
600°C
114.8 µohm-m
1400°F
46.1 µohm-in
700°C
116.4 µohm-m
1600°F
46.5 µohm-in
800°C
117.5 µohm-m
1800°F
46.7 µohm-in
900°C
118.3 µohm-m
2000°F
46.8 µohm-in
1000°C
119.1 µohm-m
Specific Heat
RT
0.096 Btu/lb-°F
RT
12.1 J/kg·°C
200°F
0.101 Btu/lb-°F
100°C
423 J/kg·°C
400°F
0.106 Btu/lb-°F
200°C
444 J/kg·°C
600°F
0.112 Btu/lb-°F
300°C
465 J/kg·°C
800°F
0.117 Btu/lb-°F
400°C
486 J/kg·°C
1000°F
0.122 Btu/lb-°F
500°C
502 J/kg·°C
1200°F
0.127 Btu/lb-°F
600°C
523 J/kg·°C
1400°F
0.131 Btu/lb-°F
700°C
540 J/kg·°C
1600°F
0.136 Btu/lb-°F
800°C
557 J/kg·°C
1800°F
0.140 Btu/lb-°F
900°C
573 J/kg·°C
2000° F
0.145 Btu/lb-°F
1000°C
590 J/kg·°C
Thermal Conductivity
RT
72 Btu-in/ft
2
-hr-°F
RT
10.4 W/m-°C
200°F
84 Btu-in/ft
2
-hr-°F
100°C
12.2 W/m-°C
400°F
100 Btu-in/ft
2
-hr-°F
200°C
14.3 W/m-°C
600°F
112 Btu-in/ft
2
-hr-°F
300°C
15.9 W/m-°C
800°F
125 Btu-in/ft
2
-hr-°F
400°C
17.5 W/m-°C
1000°F
138 Btu-in/ft
2
-hr-°F
500°C
19.3 W/m-°C
1200°F
152 Btu-in/ft
2
-hr-°F
600°C
21.1 W/m-°C
1400°F
167 Btu-in/ft
2
-hr-°F
700°C
23.0 W/m-°C
1600°F
174 Btu-in/ft
2
-hr-°F
800°C
24.8 W/m-°C
1800°F
189 Btu-in/ft
2
-hr-°F
900°C
25.5 W/m-°C
2000°F
204 Btu-in/ft
2
-hr-°F
1000°C
27.6 W/m-°C
Thermal Diffusivity
RT
4.5 x 10
-3
in
2
/sec
RT
29.2 x 10
-3
cm2/s
200°F
5.0 x 10
-3
in
2
/sec
100°C
32.7 x 10
-3
cm
2
/s
400°F
5.6 x 10
-3
in
2
/sec
200°C
36.5 x 10
-3
cm
2
/s
600°F
6.0 x 10
-3
in
2
/sec
300°C
38.7 x 10
-3
cm
2
/s
800°F
6.4 x 10
-3
in
2
/sec
400°C
40.8 x 10
-3
cm
2
/s
1000°F
6.7 x 10
-3
in
2
/sec
500°C
43.5 x 10
-3
cm
2
/s
1200°F
7.1 x 10
-3
in
2
/sec
600°C
45.7 x 10
-3
cm
2
/s
1400°F
7.6 x 10
-3
in
2
/sec
700°C
48.2 x 10
-3
cm
2
/s
1600°F
7.6 x 10
-3
in
2
/sec
800°C
50.4 x 10
-3
cm
2
/s
1800°F
8.0 x 10
-3
in
2
/sec
900°C
50.4 x 10
-3
cm
2
/s
2000°F
8.4 x 10
-3
in
2
/sec
1000°C
53.0 x 10
-3
cm
2
/s
Mean Coefficient of
Thermal Expansion
75-200°F
6.7 10
-6
in/in/°F
25-100°C
12.1 10
-6
m/m/°C
75-400°F
7.1 10
-6
in/in/°F
25-200°C
12.7 10
-6
m/m/°C
75-600°F
7.3 10
-6
in/in/°F
25-300°C
13.1 10
-6
m/m/°C
75-800°F
7.6 10
-6
in/in/°F
25-400°C
13.5 10
-6
m/m/°C
75-1000°F
7.7 10
-6
in/in/°F
25-500°C
13.9 10
-6
m/m/°C
75-1200°F
8.2 10
-6
in/in/°F
25-600°C
14.3 10
-6
m/m/°C
75-1400°F
8.5 10
-6
in/in/°F
25-700°C
15.0 10
-6
m/m/°C
75-1600°F
8.8 10
-6
in/in/°F
25-800°C
15.5 10
-6
m/m/°C
75-1800°F
9.1 10
-6
in/in/°F
25-900°C
16.0 10
-6
m/m/°C
-
-
25-1000°C
16.5 10
-6
m/m/°C
Dynamic Modulus
of Elasticity
RT
33.7 x 10
6
psi
RT
232 GPa
200°F
32.9 x 10
6
psi
100°C
226 GPa
400°F
31.8 x 10
6
psi
200°C
220 GPa
600°F
30.8 x 10
6
psi
300°C
213 GPa
800°F
29.5 x 10
6
psi
400°C
206 GPa
1000°F
28.6 x 10
6
psi
500°C
198 GPa
1200°F
27.1 x 10
6
psi
600°C
189 GPa
1400°F
25.6 x 10
6
psi
700°C
180 GPa
1600°F
24.0 x 10
6
psi
800°C
171 GPa
1800°F
22.2 x 10
6
psi
900°C
160 GPa
2000°F
20.2 x 10
6
psi
1000°C
150 GPa
Dynamic Shear Modulus
RT
13.0 x 10
6
psi
RT
90 GPa
400°F
12.5 x 10
6
psi
100°C
88 GPa
600°F
12.0 x 10
6
psi
200°C
86 GPa
800°F
11.4 x 10
6
psi
300°C
83 GPa
1000°F
10.9 x 10
6
psi
400°C
80 GPa
1200°F
10.3 x 10
6
psi
500°C
76 GPa
1400°F
9.7 x 10
6
psi
600°C
73 GPa
1600°F
9.0 x 10
6
psi
700°C
69 GPa
1800ºF
8.3 x 10
6
psi
800ºC
65 GPa
2000°F
7.5 x 10
6
psi
900°C
61 GPa
-
-
1000ºC
56 GPa
Poisson's Ratio
RT°F
0.3
RT
0.30
200°F
0.29
100°C
0.29
400°F
0.27
200°C
0.27
600°F
0.29
300°C
0.29
800°F
0.29
400°C
0.29
1000°F
0.31
500°C
0.30
1200°F
0.32
600°C
0.31
1400°F
0.32
700°C
0.32
1600°F
0.33
800°C
0.32
1800°F
0.33
900°C
0.33
2000°F
0.34
1000°C
0.33
RT = Room Temperature