Impact Strength

Product Form Condition Test Temperature Impact Strength
°F °C ft-lbf J
Plate Solution Annealed RT RT 198 268
Plate Solution Annealed -320 -196 150 203
Bar Solution Annealed RT RT 401 544
Bar Solution Annealed -320 -196 343 465
Plate Age Hardened* RT RT 91 123
Ring Annealed + Age Hardened* RT RT 51 69
*Aged hardened:  1200°F (649°C) / 24 h / Air Cool