Haynes International
Investor Relations
Customer Portal
English
日本語
中文
español
800.354.0806
765.456.6012
The Home of HASTELLOY® and HAYNES® Alloys
When autocomplete results are available use up and down arrows to review and enter to select.
Our Company
Company Overview
Locations and Directions
Investor Relations
Corporate Governance
Corporate Governance Guidelines
Corporate Policies
Human Trafficking Policy
Human Rights Policy
Conflicts Minerals Policy
Cancellation Policy
Anti-Harassment Policy
Anti-Corruption Policy
Health, Safety, Environmental, and Quality Policy
Energy Policy
Code of Business Conduct and Ethics
Suppliers and Third Party Intermediaries
EthicsPoint Whistleblower Hotline
Conduct and Ethics Compliance
Directors and Executive Officers
Composition of Board Committees
Board Committee Charters
Sustainability
Environmental
Social
Governance
Our Positive Impact
Health, Safety, Environmental, and Quality
Health, Safety, Environmental, and Quality Policy
MSDS/Safety Data Sheets
Safety Data Sheets, English
Safety Data Sheets, Chinese
Safety Data Sheets, Czech
Safety Data Sheets, French
Safety Data Sheets, German
Safety Data Sheets, Italian
Safety Data Sheets, Japanese
Safety Data Sheets, Korean
Safety Data Sheets, Spanish
Energy Policy
Accreditations and Approvals
REACh
Trademarks
Our Heritage
Our Founder, Elwood Haynes
Our Company History
Our Milestones
Our Contributions to History
Careers
News
Markets
Aerospace
Power Generation
Chemical Processing
Emerging Technologies
Other Markets
Alloys
Alloy Portfolio
High-temperature Alloys
HAYNES® 25 alloy
HAYNES® 75 alloy
HAYNES® 188 alloy
HAYNES® 214® alloy
HAYNES® 230® alloy
HAYNES® 233™ alloy
HAYNES® 242® alloy
HAYNES® 244® alloy
HAYNES® 263 alloy
HAYNES® 282® alloy
HAYNES® 556® alloy
HAYNES® 617 alloy
HAYNES® 625 alloy
HAYNES® 625SQ® alloy
HAYNES® 718 alloy
HAYNES® HR-120® alloy
HAYNES® HR-160® alloy
HAYNES® HR-224® alloy
HAYNES® HR-235® alloy
MULTIMET® alloy
HAYNES® NS-163® alloy
HAYNES® R-41 alloy
HASTELLOY® S alloy
HASTELLOY® W alloy
HAYNES® Waspaloy alloy
HASTELLOY® X alloy
HAYNES® X-750 alloy
Corrosion-resistant Alloys
HASTELLOY® B-3® alloy
HASTELLOY® C-4 alloy
HASTELLOY® C-22® alloy
HASTELLOY® C-22HS® alloy
HASTELLOY® C-276 alloy
HASTELLOY® C-2000® alloy
HASTELLOY® G-30® alloy
HASTELLOY® G-35® alloy
HASTELLOY® HYBRID-BC1® alloy
HASTELLOY® N alloy
ULTIMET® alloy
Titanium Alloy
HAYNES® Ti-3Al-2.5V alloy
Alloy Nominal Compositions
Product Forms
Sheet and Plate
Wire and Welding
Pipe and Tubing
Bar and Billet
Fittings and Flanges
Welding and Fabrication
Welding and Fabrication Overview
Wire and Welding Product Forms
Hot-working
Cold-working
Welding and Joining
Heat Treatment
Machining
Grinding
Descaling and Pickling
Welding SmartGuide
Welding and Fabrication Brochure
Corrosion Guide
Introduction
Alloy Backgrounds
Alloy Groups
Metallurgy
Corrosive Environments
Wear Background
Abrasion
Erosion
Metal‐to‐Metal Sliding Wear
Corrosion Alloy Manual
Alloy Innovation
Alloy Development
Alloy Manufacturing
Alloy Technical Support
Specifications and Codes
Accreditations and Approvals
MSDS/Safety Data Sheets
Trademarks
Technical Library
Sales and Service
Sales and Service
Sales Office and Service Center Locations
Request for Quote
Terms and Conditions of Sale
Nickel Surcharges
Cancellation Policy
Export Compliance Policy Letter
Due Diligence
Incoterms®
Alloys and Products Brochure
Processing Capabilities
Abrasive Saw Cutting
Bar Saw Cutting
Laser Cutting
Near-net Shaped Cut Parts
Plasma Cutting
Precision Shearing
Virtek® Laser QC®
Waterjet Cutting
Contact
Sales
Technical Support
Investor Relations
Careers
General Information
HASTELLOY® HYBRID-BC1® alloy
Home
Alloys
Alloy Portfolio
Corrosion-resistant Alloys
HASTELLOY® HYBRID-BC1® alloy
Physical Properties
HASTELLOY® HYBRID-BC1® alloy
Principal Features
Nominal Composition
Iso-Corrosion Diagrams
Corrosion Data
Selected Corrosion Data
Localized Corrosion Data
Effect of Oxidizing Species
Resistance to Stress Corrosion Cracking
Physical Properties
Impact Strength
Tensile Data
Heat Treatment
Forming
Specifications and Codes
Disclaimer
Alloy Brochure
ASP.sfctrlpresentation_openaccessdataprovider_7b98424546ba62e18cdfff0000376e70_ascx
HASTELLOY® HYBRID-BC1® alloy
Principal Features
Nominal Composition
Iso-Corrosion Diagrams
Corrosion Data
Selected Corrosion Data
Localized Corrosion Data
Effect of Oxidizing Species
Resistance to Stress Corrosion Cracking
Physical Properties
Impact Strength
Tensile Data
Heat Treatment
Forming
Specifications and Codes
Disclaimer
Alloy Brochure
Physical Properties
Physical Property
British Units
Metric Units
Density
RT
0.319 lb/in
3
RT
8.83 g/cm
3
Electrical Resistivity
RT
49.5 µohm.in
RT
1.26 µohm.m
200°F
49.9 µohm.in
100°C
1.2 µohm.m
400°F
50.3 µohm.in
200°C
1.27 µohm.m
600°F
50.3 µohm.in
300°C
1.28 µohm.m
800°F
50.7 µohm.in
400°C
1.28 µohm.m
1000°F
51.4 µohm.in
500°C
1.29 µohm.m
1100°F
51.9 µohm.in
600°C
1.31 µohm.m
Thermal Conductivity
RT
64 Btu.in/h.ft
2
.°F
RT
9.30 W/m.°C
200°F
72 Btu.in/h.ft
2
.°F
100°C
10.5 W/m.°C
400°F
84 Btu.in/h.ft
2
.°F
200°C
11.9 W/m.°C
600°F
95 Btu.in/h.ft
2
.°F
300°C
13.5 W/m.°C
800°F
106 Btu.in/h.ft
2
.°F
400°C
14.9 W/m.°C
1000°F
117 Btu.in/h.ft
2
.°F
500°C
16.4 W/m.°C
1100°F
121 Btu.in/h.ft
2
.°F
600°C
17.5 W/m.°C
Mean Coefficient of
Thermal Expansion
70-200°F
6.4 µin/in.°F
25-100°C
11.5 µm/m.°C
70-400°F
6.6 µin/in.°F
25-200°C
11.9 µm/m.°C
70-600°F
6.8 µin/in.°F
25-300°C
12.2 µm/m.°C
70-800°F
7.0 µin/in.°F
25-400°C
12.5 µm/m.°C
70-1000°F
7.1 µin/in.°F
25-500°C
12.7 µm/m.°C
70-1100°F
7.0 µin/in.°F
25-600°C
12.7 µm/m.°C
Thermal Diffusivity
RT
0.102 ft
2
/h
RT
0.0264 cm
2
/s
200°F
0.111 ft
2
/h
100°C
0.0291cm
2
/s
400°F
0.124 ft
2
/h
200°C
0.0319 cm
2
/s
600°F
0.138 ft
2
/h
300°C
0.0352 cm
2
/s
800°F
0.151 ft
2
/h
400°C
0.0382 cm
2
/s
1000°F
0.163 ft
2
/h
500°C
0.0412 cm
2
/s
1100°F
0.168 ft
2
/h
600°C
0.0435 cm
2
/s
Specific Heat
RT
0.096 Btu/lb.°F
RT
403 J/kg.°C
200°F
0.099 Btu/lb.°F
100°C
416 J/kg.°C
400°F
0.102 Btu/lb.°F
200°C
429 J/kg.°C
600°F
0.105 Btu/lb.°F
300°C
439 J/kg.°C
800°F
0.108 Btu/lb.°F
400°C
449 J/kg.°C
1000°F
0.110 Btu/lb.°F
500°C
461 J/kg.°C
1100°F
0.109 Btu/lb.°F
600°C
457 J/kg.°C
Dynamic Modulus of
Elasticity
RT
31.5 x 10
6
psi
RT
217 GPa
200°F
30.7 x 10
6
psi
100°C
211 GPa
400°F
29.8 x 10
6
psi
200°C
205 GPa
600°F
28.9 x 10
6
psi
300°C
200 GPa
800°F
28.3 x 10
6
psi
400°C
197 GPa
1000°F
27.5 x 10
6
psi
500°C
191 GPa
1200°F
27.0 x 10
6
psi
600°C
188 GPa
Poisson’s Ratio
-
-
RT
0.33
RT= Room Temperature