Physical Properties

Physical Property British Units Metric Units
Density RT 2.97 lb/in3  RT 8.22 g/cm3
Electrical Resistivity RT RT RT 1.16 μohm.m
200°F 200°F 100°C 1.17 μohm.m
400°F 400°F 200°C 1.19 μohm.m
600°F 600°F 300°C 1.21 μohm.m
800°F 800°F 400°C 1.23 μohm.m
1000°F 1000°F 500°C 1.24 μohm.m
- - 600°C 1.25 μohm.m
Thermal Conductivity RT RT RT 10 W/m.°C
200°F 200°F 100°C 12 W/m.°C
400°F 400°F 200°C 14 W/m.°C
600°F 600°F 300°C 17 W/m.°C
800°F 800°F 400°C 19 W/m.°C
1000°F 1000°F 500°C 20 W/m.°C
- - 600°C 21 W/m.°C
Mean Coefficient of
Thermal Expansion
86-200°F 86-200°F 30-100°C 12.8 μm/m.°C
86-400°F 86-400°F 30-200°C 13.8 μm/m.°C
86-600°F 86-600°F 30-300°C 14.3 μm/m.°C
86-800°F 86-800°F 30-400°C 14.8 μm/m.°C
86-1000°F 86-1000°F 30-500°C 15.3 μm/m.°C
86-1200°F 86-1200°F 30-600°C 15.8 μm/m.°C
Dynamic Modulus
of Elasticity
RT RT RT 202 GPa
400°F 400°F 200°C 196 GPa
600°F 600°F 300°C 195 GPa
800°F 800°F 400°C 192 GPa
1000°F 1000°F 500°C 187 GPa

RT= Room Temperature