Form |
Test
Temperature |
Thickness/Bar Diameter |
0.2% Offset
Yield Strength |
Ultimate
Tensile Strength |
Elongation |
°F |
°C |
in |
mm |
ksi |
MPa |
ksi |
MPa |
% |
Sheet |
RT |
RT |
0.028-0.125 |
0.7-3.2 |
59 |
407 |
116 |
800 |
57 |
Sheet |
200 |
93 |
0.028-0.125 |
0.7-3.2 |
54 |
372 |
110 |
758 |
58 |
Sheet |
400 |
204 |
0.028-0.125 |
0.7-3.2 |
44 |
303 |
102 |
703 |
57 |
Sheet |
600 |
316 |
0.028-0.125 |
0.7-3.2 |
42 |
286 |
98 |
676 |
62 |
Sheet |
800 |
427 |
0.028-0.125 |
0.7-3.2 |
41 |
283 |
95 |
655 |
67 |
Sheet |
1000 |
538 |
0.028-0.125 |
0.7-3.2 |
40 |
276 |
91 |
627 |
61 |
Sheet |
1200 |
649 |
0.028-0.125 |
0.7-3.2 |
36 |
248 |
85 |
586 |
65 |
Sheet |
1400 |
760 |
0.028-0.125 |
0.7-3.2 |
35 |
241 |
76 |
524 |
63 |
Plate |
RT |
RT |
0.25-0.75 |
6.4-19.1 |
54 |
372 |
114 |
786 |
62 |
Plate |
200 |
93 |
0.25-0.75 |
6.4-19.1 |
49 |
338 |
107 |
738 |
65 |
Plate |
400 |
204 |
0.25-0.75 |
6.4-19.1 |
41 |
283 |
98 |
676 |
66 |
Plate |
600 |
316 |
0.25-0.75 |
6.4-19.1 |
36 |
248 |
95 |
655 |
68 |
Plate |
800 |
427 |
0.25-0.75 |
6.4-19.1 |
35 |
241 |
92 |
634 |
68 |
Plate |
1000 |
538 |
0.25-0.75 |
6.4-19.1 |
34 |
234 |
88 |
607 |
67 |
Plate |
1200 |
649 |
0.25-0.75 |
6.4-19.1 |
32 |
221 |
83 |
572 |
69 |
Plate |
1400 |
760 |
0.25-0.75 |
6.4-19.1 |
31 |
214 |
76 |
524 |
68 |
Bar |
RT |
RT |
0.5-2.0 |
12.7-50.8 |
52 |
359 |
111 |
765 |
70 |
Bar |
200 |
93 |
0.5-2.0 |
12.7-50.8 |
45 |
310 |
105 |
724 |
73 |
Bar |
400 |
204 |
0.5-2.0 |
12.7-50.8 |
38 |
262 |
96 |
662 |
74 |
Bar |
600 |
316 |
0.5-2.0 |
12.7-50.8 |
34 |
234 |
92 |
634 |
79 |
Bar |
800 |
427 |
0.5-2.0 |
12.7-50.8 |
31 |
214 |
89 |
614 |
79 |
Bar |
1000 |
538 |
0.5-2.0 |
12.7-50.8 |
29 |
200 |
84 |
579 |
80 |
Bar |
1200 |
649 |
0.5-2.0 |
12.7-50.8 |
28 |
193 |
80 |
552 |
80 |
Bar |
1400 |
760 |
0.5-2.0 |
12.7-50.8 |
29 |
200 |
72 |
496 |
77 |
Values are averages from numerous tests
RT= Room Temperature